I have a black powder that I cannot reliably tell just by looking or touching whether it is graphite powder or charcoal powder.

Are there any simple tests that I can perform to tell whether it is one or the other?

What I have tried:

  • Adding it to water, it sinks to the bottom and leaves a slight oily looking film on the top. Upon stirring, it darkens the water and then gradually sinks back to the bottom after some time.

  • I tried writing some thick lines on a piece of paper with a graphite pencil and testing for conductivity (high resistance).

  • Same high resistance with the powder (granted this is very unrepeatable)

  • Rubbing it into paper it has a much blacker colour than the graphite (which to me looks like a really dark gray). However, I don't know if that is a reliable indicator.

I've also added a picture, if it helps:

carbon powder


EDIT:

Ok, I've made a paste using isopropyl alcohol and the carbon powder and made a small "stick" or rod of the stuff. I have now been able to achieve solid continuity at around 2 centimeters in distance and the resistance dropped from the high 40 - 50 kOhms for the loose powder, to the low 10s (ie 40 Ohms). If this helps anyone.

enter image description here

$\endgroup$
5
  • $\begingroup$ Well, x-ray crystallography would work, but I suppose you're looking for some other way ;) $\endgroup$ Nov 9 '17 at 15:56
  • 2
    $\begingroup$ Besides, I'm inclined to believe that a given sample of charcoal is not 100% amorphous carbon, and that a given sample of graphite is not 100% crystalline either. So asking whether this sample is "graphite" or "charcoal" poses other issues... $\endgroup$ Nov 9 '17 at 15:59
  • $\begingroup$ Yeah, I guess a question about the particular alotrope of carbon you have in your hand is perhaps much for "simple experiments". $\endgroup$
    – made2hack
    Nov 9 '17 at 16:12
  • $\begingroup$ No idea beside conductivity test . If you have access to Raman it would be rather simple to discriminate between mostly charcoal or mostly graphite. $\endgroup$
    – Alchimista
    Nov 9 '17 at 16:55
  • $\begingroup$ Ok, when I test for conductivity, I get a good reading from the pencil led, max 30 Ohm. However, when I test for conductivity for the lines drawn on the paper, I don't get the beep since it's like 50kOhm resistance. Same for the powder, I get high resistance since it is not exactly a cohesive structure if you will. $\endgroup$
    – made2hack
    Nov 9 '17 at 17:00
8
$\begingroup$

Short answer: You can't reliably tell the "difference" (by any simple means)


Longer version:

First of all, the graphite you were taught about at school is a pedagogical construct. Any macroscopic sample of "real" graphite would contain both the layered honeycomb (crystalline) bits as well as amorphous bits of carbon (in addition to God-knows-what bunch of other substances that managed to wiggle their way into your sample).

What about charcoal then? It's amorphous carbon with significant quantities of several kinds of organic compounds (you can't expect them all to decompose to carbon...), depending on the source.

Trying to class your sample (which clearly has other stuff in it... I can see white/gray specks on it in the first picture ;P) as "graphite" or "charcoal" is an effort in futility; neither "real" graphite nor charcoal have a sharply defined constitution.

Simple tests of the physical nature of the powder would not be able to accurately distinguish it from being "mostly graphite" or "mostly charcoal", mainly, because it's a powder. Had you had the sample before it was pulverized you could (easily) tell the difference; the qualities that most people attribute to graphite (luster, slippery-ness) aren't easily discernible when you turn it into a powder and then compare it with powdered charcoal.


About the tests you conducted:

Your attempt to subject the sample to various (physical) tests is laudable (more users ought to do that before posting "Identify this thingy"-type questions here... it may give us something to work with). However those tests, apart from sorely lacking in some sort of mechanism/procedure to cut down on sources of error, don't really provide any meaningful data that you or me or anyone could use to determine what your sample is (largely) composed of.

Let's break down what you did

  • Adding it to water, it sinks to the bottom and leaves a slight oily looking film on the top. Upon stirring, it darkens the water and then gradually sinks back to the bottom after some time.

The film isn't really a giveaway. Even particles denser than water are known to "float" in these circumstances... well, they aren't technically "floating", it's the surface tension of the water that's holding it up. This is easily disrupted by stirring/agitation, and as you've noticed, it'll sink.

Graphites typically have have a much higher density (slight variation depending on purity and crystal defects) than water, so pieces of "graphite" would sink.

Blocks of charcoal typically have lower densities (varies depending on type/source of charcoal) than water and hence floats, but that changes when you pulverize them (and destroy most of the air cavities in the process).

Conclusion: No useful data.

  • I tried writing some thick lines on a piece of paper with a graphite pencil and testing for conductivity (high resistance).

  • Same high resistance with the powder.

That was a lot of effort... for nothing (you have my deepest sympathies).

Okay, I think I see your reasoning here:

"Graphite's pretty conductive (low-ish resistance) and charcoal is a poor conductor (very high resistance), so doesn't this test tell me something?"

Nope.

Thing about pure graphite (of the "Holy cow! A non-metal that conduct electricity!!!" fame) is that it only conducts (really well) along a particular plane; try another plane perpendicular to this and you'll find it to be a thousand times less conductive ( see answer to this question).

Even if your powder is (largely) graphite, surely the individual powder particles aren't going to align themselves into an extended plane between your terminals. They'll be oriented randomly, so expect the high resistance.

You first drew a line on a piece of paper using a pencil and measured its resistance to create a baseline to work up from. Smart. Just two things though:

  • 1) Pencil lead isn't graphite (neither is it "lead" for that matter ;P); it's a mixture of graphite and clay. So unless you know for sure that the impurities in your sample are clay, this doesn't really serve as a good baseline. Besides, the graphite particles aren't all aligned in that plane I was talking about.

  • 2) Your makeshift resistor ("thick line on a piece of paper") is a poor standard for another reason: dimensions. Your line has no uniform dimensions (length, breadth or even depth). If you need resistance from resistivity of a given material, or the other way around, you need the sample's dimensions. Neither your line nor your powder have fixed dimensions in this test.

Trying to figure out what your sample is by comparing its resistivity with that of another substance is a really neat idea, so don't get me wrong; the issue here is (1) the design of the experiment, (2) of the two substances you're trying to compare (graphite and charcoal), the latter's electrical properties are altered because it's been powdered and (3) your "control-test/sample" (the line-resistor) is neither graphite nor charcoal, making it a rather pointless "control sample".

Conclusion: No useful data.

  • Rubbing it into paper it has a much blacker colour than the graphite (which to me looks like a really dark gray). However, I don't know if that is a reliable indicator.

I don't need to tell you how poor a test this is (you already seem to doubt the validity of the test yourself)

Conslusion: No useful data.

  • EDIT: Ok, I've made a paste using Isopropyl Alcohol and the carbon powder and made a small "stick" or rod of the stuff. I have now been able to achieve solid continuity at around 2 centimeters in distance and the resistance dropped from the high 40 - 50 kOhms for the loose powder, to the low 10s (ie 40 Ohms). If this helps anyone.

Same argument as before: This test is pointless because your sample doesn't have fixed, uniform dimensions. Nor do the particles (if they're graphite; doesn't matter if it's charcoal) align themselves in extended planes.

As for the drop in resistance, I reckon it's because the sample isn't completely dry. The "isopropanol" you get at the drugstore is at least one-quarter water (not pure isopropanol). After you mixed it with your sample, a ton of electrolytes would've dissolved in the water (pretty sure your sample has loads of stuff that isn't carbon/ carbon-based). When you measured the resistance across this stick of yours, all that water hadn't evaporated by then. This is probably the (main) reason for the drop.

Conclusion: No useful data.


Interesting question by the way, you have my upvote ;)

$\endgroup$
2
  • 1
    $\begingroup$ Even bigger question: is there any point on the continuum where there is a clear dividing line between highly impure charcoal and relatively pure graphite when both exist as fine powders? I'm not sure there is. $\endgroup$
    – matt_black
    Nov 10 '17 at 15:27
  • 3
    $\begingroup$ @paracetamol - Thanks for all your input. I will definitely accept this answer as it does an awesome job of clarifying my muddied water. As for the isopropanol, I used tech grade (99.1%). $\endgroup$
    – made2hack
    Nov 11 '17 at 14:42
2
$\begingroup$

The first thing I would try would be to tie a length of thread to the ceiling and attach a non-magnetic sample holder to the free end. Put your sample in the holder and see how much you can deflect it from vertical with a strong pyramid magnet such as https://supermagnetman.com/collections/neodymium/products/pyr1000n . (If it's inappropriate to link to vendor sites please feel free to edit this out.) Graphite is one of the more diamagnetic substances (although far short of superconductors), so it should deflect more than an equivalent mass of charcoal. For comparison you could get some pyrolytic graphite, a 1 in X 1 in X 6 mm block is about $50 I think, break (or cleave) a little chunk off and grind it up so you would have a good graphite standard for comparison. They are fun toys to have around and worth it not just for the sake of this experiment.

$\endgroup$

Your Answer

By clicking “Post Your Answer”, you agree to our terms of service, privacy policy and cookie policy

Not the answer you're looking for? Browse other questions tagged or ask your own question.